Abrasion is a major factor in the R&D stage of fabrics. In fabric testing laboratories, abrasion tests predict fabric’s durability in real-world use. In this article, we will thoroughly introduce ISO 12947, a standard for testing abrasion using the Martindale method, including details of its subparts, working principles, apparatus, and experiences from technicians.
What is Fabric Abrasion?
The wear and tear of a material due to frictional contact with another surface is called abrasion. Abrasion is one of the most common problems of any fabric.
Abrasion and Its Impact
Abrasion affects fabrics in several ways.
- It can change the appearance of the fabric. i.e., can fade or change color.
- If the fabric is abraded sheerly, it can lose its fibers, causing weight loss.
- Highly intense abrasion can even cause holes or tears in the fabric.
Abrasion Resistance Standards
ISO 12947 and its different parts
ISO 12947 is an international standard for testing abrasion and is used worldwide. It consists:
- ISO 12947-1 – Martindale Abrasion Testing Apparatus
- ISO 12947-2 – Determination of Specimen Breakdown
- ISO 12947-3 – Determination of Mass loss
- ISO 12947-4 – Assessment of Appearance change
All parts have nearly the same testing procedure and testing conditions. The difference lies in the evaluation method.
What is the difference between Abrasion and Pilling?
Pilling and abrasion are often described as the same processes but differ. Abrasion is the frictional wear and tear that another substance causes on fabric, resulting in a change in appearance, loss in fabric weight, and deformation of fabric. Pilling is the fuzziness on the fabric’s surface due to friction. It causes the ball formation of protruding fibers.
Methods used for Abrasion Resistance
In addition to ISO 12947, other standards are used worldwide for abrasion. Following is a list of such standards
- ASTM 4966
- FZ/T98014
- GB/T13775
Working principle of ISO 12947
A circular fabric sample is rubbed with the same fabric or a standard wool abradant cloth at a constant force in a Lissajous pattern. The specimen holder containing specimen or abrasive medium depends on which part of ISO 12947 is used. The test sample is freely moved around its axis through its center. Fabric abrasion, weight loss, or appearance change are visually examined after the test.
Martindale Pilling Tester

The Martindale test apparatus is used both for pilling and abrasion. It has various components, including a base plate that houses the pilling tables and drive mechanism. The drive system’s two outside drives and inner drive cause the sample holding plate to create a Lissajous figure. The sample test holder plate is moved horizontally using a driving mechanism for each guide plate point to exhibit the same pattern.
The Lissajous movement is a pattern produced by changing movement from a circle to a narrowly contracting ellipse until a straight line is formed. It is repeated diagonally. When one of the outer drives rotates, a pre-settable counting device built within the apparatus considers it a revolution. One revolution is regarded as one rub, and after the 16-revolution, the Lissajous pattern is formed completely.
Testing conditions of Sample
Conditioning of samples required specific standard atmospheric conditions as described in ISO 139 (20 ± 2°C Temperature and 65± 2% Relative Humidity)
Identification of face fabric
- Use an identification mark on each sample.
- Identification will help during the evaluation that all samples have a front side.
The procedure of ISO 12947
ISO 12947-1
This method describes how to test with the Martindale Testing Apparatus. It describes the Martindale Abrasion Tester, specimen, and standard fabric sizes for upper and lower plates. It also tells about foam and felt used in ISO 12947-2, ISO 12947-3, and ISO 12947-4.
Apparatus
- Martindale Abrasion Tester.
- Fabric cutters with diameters 140mm and 38 mm.
- Fabric Sample with 140 mm diameter.
- Felt for fabric Sample having 140 mm diameter.
- Abradant fabric with 38 mm diameter.
- Abradant foam with 38 mm diameter.
- Light Box with different light sources, including D-65, C.W.F, and TL-84.
- Photo Graphic Standards
- Mounting Weight
ISO 12947-2
This method specifies the procedure for sample breakdown by evaluation at fixed revolutions.
In this method, the fabric sample is rubbed with a standard fabric. In the end, the fabric is inspected for any sample breakdown.

Procedure
- Place the sample on a mounting plate by inserting felt and fabric specimens. Tight the nut once completed.
- Similarly, place the abradant fabric on an upper plate by first inserting foam.
- Ensure the face of the fabric is exposed to the specimen.
- Mount the weight for even pressure.
- Start the Martindale tester for the test.
- Note the number of revs at which specimen breakdown is not started. This number shows the maximum value of its resistance. Also, note the tester’s revs at which the sample breaks down. It shows the lower limit.
ISO 12947-3
This method deals with losing weight of fabric due to abrasion.
In this method, the fabric sample is rubbed with a standard fabric. In the end, the fabric is evaluated by the difference in weight before and after the test.
Procedure
- Mount the sample on a mounting plate by inserting felt and fabric specimens. Tight the nut once completed.
- Similarly, place the abradant fabric on an upper plate by inserting foam.
- Ensure the face of the fabric is exposed to the specimen.
- Mount the weight for even pressure.

- Start the tester by entering the required number of revolutions for the test.
- Abrade the specimens to selected test intervals.
- Weight the specimen as prescribed and remount with care.
- Continue the test until all revolutions are finished.
ISO 12947-4
This method deals with changes in fabric appearance due to abrasion. The appearance change of the fabric is evaluated by comparing it with the original fabric. It can be done in 2 ways:
- By the number of agreed revolutions
- By an agreed fabric surface change
Procedure
- Place the sample on a mounting plate by inserting felt and fabric specimens. Tight the nut once completed.
- Similarly, place the abradant fabric on an upper plate by inserting foam.
- Ensure the face of the fabric is exposed to the specimen.
- Mount the weight for even pressure.
- Start the tester by entering the required number of revolutions for the test.
- Examine the specimen after the 16 and then after every 8 rubs.
- Continue the test until the desired revolutions are covered.
Reporting Results
Prepare a test report containing the following parameters
- Fabric sample detail (type of yarn, blend ratio, woven or knit)
- Pretreatment processes (washed or dry-cleaned)
- Number of test samples
- Number of revolutions
- Type of Abradant used
- Mounting load weight i.e., 9 kpa or 12 kpa
- For ISO 12947-3, show results w.r.t revolutions. Determine the loss of mass against prescribed intervals. Use the difference of mass loss before and after the test and calculate the mean value.
- For ISO 12947-4, use each sample’s grading scale system. If grading is in between two grades, use mean values; e.g., if the value is in between grades 5 and 4, use 4-5.
Grade 5 – No change in surface
Grade 4 – Slightly
Grade 3 – Moderate Pilling
Grade 2 – Severe Pilling
Grade 1 – Very Severe Pilling
- Mention the ISO part under which the test is performed.
- Date of test performance
Practical experiences and insights
- If the total effective weight of the abrasion load (weight of specimen + holder assembly) is (795 ± 7 g), use the pressure of 12 kpa.
- If the total effective mass of the abrasion load is (595 ± 7 g), use the pressure of 9 kpa.
- Specimens with a GSM of more than 500 are mounted without foam backing.
- Use a new abradant for each test. For abrasion tests having 50,000 revs or greater, replace the abradant after every 50,000 revolutions.
- Test specimens should be taken from different locations. No sample should share the same thread.
- If a sample has less GSM, caution that the specimen should not be visibly stretched.
- While evaluating in the lightbox, view the sample from just outside the lightbox. It will stop the glare in the eyes.
- Try to evaluate with two or more observers due to differences in opinion.
Conclusion
In the textile industry, ISO 12947 is a frequently used standard, the benchmark for Martindale abrasion testing to evaluate the fabric’s lifespan. This test is important in the physical testing of fabric. It helps manufacturers to maintain better quality and needs according to end users. It also shows that fabrics are durable and have longevity. This ultimately leads to increased customer satisfaction and sales of garments.
Explore DaRong’s Martindale Abrasion Tester!
FAQs
What are the ISO and ASTM standards for abrasion?
ISO 12947-1, 12947-2, 12947-3, and 12947-4 are the ISO standard for abrasion testing. ASTM 4966 also deals with abrasion of fabric. These standards are used to keep things in a straight line.
Can we prevent abrasion?
Mostly, it is hard, especially with certain fabrics and items. Abrasion is always feasible to some extent. There are some ways to control abrasion. One of them includes washing the garment’s inner surface out while washing. Usually, garment care labels have washing instructions from the manufacturer. Follow these instructions.
Can we improve the abrasion resistance of the fabric?
Abrasion is a complicated process since it is affected by several technical factors that define the quality of fabrics—a few of these factors are described below.
- Fiber Blending
A blend of stronger fibers increases the abrasion resistance. You can improve the abrasion resistance by combining fibers such as polyester and nylon.
- Special Finishes
The fabric finishing method has a major impact on the level of abrasion—the fabric’s surface changes after finishing, which also impacts abrasion. Friction can be reduced by applying coatings or special finishes, which add a protective layer over the fabric.
- Fabric Construction
Increased cloth factor and tighter weaves can both enhance resistance.
Related Resources
Ultimate Guide to Martindale Test
A Complete Guide to ASTM D4966 ISO 12947 Martindale Abrasion Test Method
Martindale Troubleshooting Guide-5 Common Problems and How to Fix Them