How to Test Textile Formaldehyde

How to Test Textile Formaldehyde

In this article, we will demonstrate how to test textile formaldehyde using DaRong’s YGB201G Formaldehyde Tester for textiles.
This test follows the standard GB/T 2912.1 — Determination of Formaldehyde — Water Extraction Method.
Begin by sampling. Cut two pieces from the fabric sample, shred them, and weigh 1 gram.
Place the shredded sample into an Erlenmeyer flask.
Measure 100 ml of distilled water and pour it into the flask containing the sample.
Seal the flask with a cap and ensure the sample is fully immersed.
Place the flask into a thermostatic water bath shaker. Shake at 40°C for 60 minutes.
After 60 minutes, remove the flask and allow it to cool to room temperature for extraction.
Set up the filter. Extract the sample solution and filter it through the filter apparatus.
Use a dropper to take 5 ml of the filtered sample solution and place it into a glass container.
Then, draw 5 ml of Nash reagent and mix it with the sample solution. Seal the container.
This is the test solution.
At the same time, prepare a reference blank by mixing 5 ml of distilled water with 5 ml of Nash reagent.
This is the reagent blank.
Place both the test solution and reagent blank into a water bath at 40°C for color development for 30 minutes.
After 30 minutes, remove the samples.
Cool them in a dark room at room temperature for another 30 minutes.
Switch on the instrument power.
Set the wavelength to 412 nm and allow the instrument to warm up.
Click “Parameter Setting.”
Set the test parameters according to the standard and customer requirements: sample mass, extraction volume, dilution factor, and number of samples.
Select “Absorbance” as the test mode.
After setting is complete, click “Save.”
Enter the absorbance test interface.
Select the testing position.
Place the cuvettes into the cuvette holder with the transparent side facing the light source.
Close the chamber door.
Click “Test” and wait for the light source to stabilize.
The instrument will automatically detect absorbance.
Choose cuvettes with similar absorbance values for the test.
Click “Parameter Setting,” select the test method, and save.
Enter the test interface.
Pour the test solution and reagent blank into their respective cuvettes.
Seal with lids and insert them sequentially into the cuvette holder.
The first position is for the reagent blank; the rest are test samples.
Close the chamber door.
Click “Test” and wait for the light source to stabilize.
The instrument will automatically measure the formaldehyde content.
After the test is complete, click “Data Search,”
Select the group number,
View the detailed results,
And print the report.
Repeat the same procedure for the remaining samples and print the results.

Click to learn about the procedures of AATCC, ASTM, ISO, etc.

Cl

Related Resource

Formaldehyde in Clothing-A Lab Tester to Boost Your Brand Value

    Scroll to Top

    ASK FOR A QUOTE

    We will contact you in one working day. Please pay attention to the email with suffix @darongtester.com