ASTM D737: Practical Tips on Air Permeability of Textile Fabrics Test Method

We are going to learn how to perform the ASTM D737 test on fabrics using the most advanced Darong YG(B)461G tester, and we will understand its requirements, including testing conditions, pressure differential, test area, nozzle selection, reporting units, unit conversion, edge leakage, abnormal results, and troubleshooting, with practical lab guidance and a real-test case study for the most accurate and repeatable measurements.

YGB461G Fabric Air Permeability Tester
YGB461G Fabric Air Permeability Tester

What Is ASTM D737 Air Permeability Testing?

ASTM D737 is the standard test method for measuring the air permeability of fabric, and its scope includes woven, knitted, nonwoven, layered, pile, and other textile materials, including coated and treated materials. This standard method is used to assess fabric performance in various applications, such as clothing, filtration, airbag fabrics, tents, and other applications where airflow matters.

Air permeability is the volume of air passing through a defined area of the testing specimen per unit time and it is expressed relative to the exposed test area.

Which Standard, Methods or Testing Instrument Should You Select?

Testing RequirementAppropriate Standard choiceImportant Test consideration
Textile fabric testing under ASTM requirementsASTM D737Follow the specified edition and customer requirements.
Testing under international fabric-air-permeability requirementsISO 9237Use the specified pressure differential and test area.
Testing according to a Chinese national methodGB/T 5453Verify the applicable edition and contract requirements.
Measuring fabric airflow using an electronic testerDaRong YG(B)461GConfirm the selected settings, measuring range, and applicable method.
Measuring very low airflow or highly resistant materialsA suitable low-flow-capable method and instrument configurationConfirm the instrument’s validated lower measuring limit before testing.

Please note that these testing methods are related but should never automatically be treated as interchangeable. The ISO 9237 Testing Standard and ASTM D737 each have their own procedural requirements; always select the testing method specified by the buyer, product specification, or test requirements rather than choosing the easiest settings.

Test Area, Pressure Differential and Conditioning

Please note that the following three variables must be documented before comparing the testing results.

Testing Area

The exposed testing area of the specimen determines the area over which airflow is measured. Always confirm the test area required by the selected method and the instrument’s actual configuration, and never assume that each nozzle or test head represents the same area.

Pressure Differential

The pressure difference across the test specimen drives the overall airflow, and ASTM D737 and ISO 9237 should not be assigned the same settings without first verifying their requirements. The pressure must come from the applicable testing standard, customer specification, or approved testing procedure.

Conditioning of the Testing Specimen

Always condition the testing specimen in the atmosphere required by the applicable testing standard. ASTM D737 references the standard atmosphere for textile testing and follows ASTM D1776, and ISO 9237 always refers to ISO 139. Record both the actual temperature and relative humidity of the testing specimen, along with the agreed deviation.

To get repeatable results, also record the specimen identification, fabric construction, number of test locations, instrument identification, and any special preparation.

How to Perform the Testing While Using Darong YG(B)461G

The Darong YG(B)461G air permeability tester features an electronic interface, selectable testing methods, and automatic airflow measurement. Always follow the instrument manual and the applicable test method to ensure an accurate operating sequence.

Prepare the Testing Specimen

Condition the testing specimen as per requirements and always avoid stretching, creasing, or contamination.

Select the Test Setting

First confirm the required testing method, pressure differential, test area, and reporting unit.

Choose the Appropriate Measuring Range

Select the nozzle or orifice configuration that can measure the expected airflow within its validated range.

Mount the Testing Specimen

Place the testing specimen properly flat over the test opening and clamp it very securely without distorting its structure.

Properly Placed Testing Specimen
Properly Placed Testing Specimen

Check the Seal

Always ensure 100% that the air cannot bypass the specimen around its edges.

Testing Area Having Excellent Sealing Properties
Testing Area Having Excellent Sealing Properties

Run the Test

Start the measurement and allow the tester to complete its measurement cycle.

Repeat at the Required Locations

Take 4 test specimens from the fabric’s test location.

Record and Review the Results

Check the reading on the screen, units, testing conditions, and any warnings before preparing the test report.

Tocuh Screen Disply Having Menu Setting and Unit Conversions Options
Tocuh Screen Disply Having Menu Setting and Unit Conversions Options

Understanding Area-Normalized Units and Their Conversion

Selection of the Result Units
Selection of the Result Units

Please always report the air permeability result with the correct unit, and the common units are:

  • cm³/(s·cm²)
  • L/(s·m²)
  • ft³/(min·ft²), usually written as CFM/ft²

The useful conversions of these units are included

  • 1 cm³/(s·cm²) = 10 L/(s·m²)
  • 1 CFM/ft² ≈ 5.08 L/(s·m²)
  • 1 CFM/ft² ≈ 0.508 cm³/(s·cm²)

For example: Result of the 25 cm³/(s·cm²) is equivalent to the 250 L/(s·m²).  Please note that this is a unit conversion example, not a measured Darong test result.

Troubleshooting of Abnormal Results

Observed Testing problemPossible causesBest recommended action
Unexpectedly high readingEdge leakage, damaged specimen, or incorrect settingsInspect the specimen and seal; verify the selected method.
Unexpectedly low readingWrong range, blocked airflow path, or highly resistant fabricCheck the setup, instrument condition, and measuring limits.
Unstable readingsPoor clamping, fabric variation, or unstable operating conditionsRemount the specimen and repeat according to the procedure.
Reading outside the instrument rangeIncorrect nozzle selection or specimen outside the measurable rangeFollow the manual for range selection; do not extrapolate an invalid result.
Large differences between locationsGenuine fabric nonuniformity or inconsistent specimen handlingTest additional locations as permitted and report variation appropriately.

Abnormal readings do not automatically indicate a failure of the test. First, determine whether the result is valid. If the seal, setting, or instrument status is incorrect, correct the issue, repeat the test, and retain the original record, documenting the reason for invalidating or repeating measurements.

Real Laboratory Case Study

ItemsLaboratory internal record
Fabric material and constructionTo be supplied from the actual test
InstrumentDarong YG(B)461G
Test standard and editionTo be confirmed from the test record
Pressure differential and test areaActual settings to be recorded
Conditioning conditionsActual laboratory conditions
Individual readings and unitsInsert verified instrument results
Mean and variation, if requiredCalculate from valid readings
InterpretationCompare against the relevant customer requirement

What Should an Air Permeability Test Report Include?

An authentic lab report identifies the fabric, testing method and edition, instrument, pressure differential, test area, conditioning conditions, individual readings if applicable, final mean result, reporting units a,nd the relevant statistical information a,nd any deviation from the specified procedure must be recorded.

When comparing testing results from different labs, use comparable methods and conditions. ASTM D737 notes that significant interlaboratory differences may require comparative testing to investigate possible bias. Read the ASTM D737 Standard Information.

Conclusion

Reliable permeability testing always requires more than operating a tester and following the correct standard; pressure differential, exposed area, conditioning, specimen sealing, measuring range a,nd reporting units matter. Darong YG(B)461G has all the related settings per the testing standard. For details on the equipment, visit the DaRong YG(B)461G product page.

FAQs

Is air permeability the same as air?

The simple answer is no. Air permeability measures the airflow through a fabric, and breathability can also involve moisture vapor transport and moisture management

Can ASTM D737 and ISO 9237 results be compared directly with each other?

Not automatically; always verify the testing conditions, exposed area, pressure differential, and the procedures before comparing the test results.

What should I do if the tester displays an out-of-range result?

Check the setup and the specimen seal, then follow the instrument manual to select an appropriate measuring range, and do not report invalid or extrapolated readings as a valid measurement.

Related Resources

Air Permeability VS Water-Vapor Permeability

Air Permeability Tester

An Ultimate Guide to Air Permeability of Fabric

Insights and Experience on ISO 9237 Fabric Air Permeability Test

    Scroll to Top

    ASK FOR A QUOTE

    We will contact you in one working day. Please pay attention to the email with suffix @darongtester.com