In a textile lab or fabric laboratory, fabric-breaking strength testing (also referred to as tensile strength testing) is an important process that decides a fabric’s strength and longevity. As a manufacturer or fabric R&D person, if you wish to ensure that the fabrics meet specific quality standards you will need to know about tensile testing. The strip method and the grab method are the two primary methods. They have positive and negative aspects. Which one to choose relies on the particular test requirements. After reading this article, you will have a thorough understanding of breaking strength and elongation as well as knowledge on how to perform ASTM D5035.
Breaking Strength and Elongation of Textile Fabrics
There are 3-types of fabric strength
- Tear
- Tensile
- Bursting
Breaking strength is also called tensile strength. It is known as the maximum tensile force when a specimen is stretched to a breaking point. It is one of the key criteria used to evaluate fabric quality. The UTM testing (Universal Testing Machine), also known as fabric tensile test device, is an electromechanical instrument to measure tensile strength that exerts a tensile force for a fabric tensile test to measure its tensile strength and deformation properties until breakage. Universal Testing Machine test procedure includes a tension or compression test in which the sample is positioned between the two jaws of the machine and tightly bound.
Fabric strength testing is crucial in the textile industry to guarantee the functionality and longevity of finished garments. The mechanical characteristics of textiles, such as their capacity to bend and resist external forces, are essential in defining their overall durability and ability to withstand damage. Furthermore, these characteristics are critical for evaluating the degree to which textiles can tolerate the various stresses and strains they endure during use.
An overview of ASTM D 5035
The most recent version of ASTM D5035, ASTM D5035 11, is named ” Standard Test Method for Breaking Force and Elongation of Textile Fabrics (Strip Method)”. It also has an old edition ASTM D5035 95. For the most accurate and up-to-date testing criteria and procedures, referring to the latest edition is recommended.
The strip method, also known as the raveled strip method, involves cutting a strip of fabric from the material being tested. The strip is clamped in a tensile testing machine and stretched until it breaks. Values for the breaking force and elongation can be taken from a computer interfaced with the testing machine. This test method concludes how to conduct fabric tensile tests using four different specimen and three different testing machine types. Use the following system to identify particular specimen and machine combinations for textile lab reports.
ASTM D5035 Sample sizes:
- 1C—25 mm (1.0 in.) cut strip test
- 2C—50 mm (2.0 in.) cut strip test
- 1R—25 mm (1.0 in.) raveled strip test
- 2R—50 mm (2.0 in.) raveled strip test
Moreover, this test can be performed on the following tensile testing devices:
- L—constant-rate-of-load (CRL)
- T—constant-rate-of-traverse (CRT)
- E—constant-rate-of-extension (CRE)
For example, 1C-E indicates a tensile test with a constant rate of extension along with a cut strip test of 25 mm (1 in.).
Knitted textiles are not advised to be tested by this method due to their stretch (if the stretch is more than 11%). The raveled strip test is ideal for woven fabrics, whereas the cut strip test is for nonwoven, felted, dipped, or coated materials.
Since the entire width of the strip is tested, one of the primary benefits of the strip method is that it gives a more realistic depiction of the fabric’s strength. However, since the fabric must be precisely cut into strips of a certain size, this procedure can take some time.
In the grab test based on ASTM D5034, a piece of cloth is clamped into the tensile testing machine without being cut into strips. After that, the machine exerts force on the fabric until it breaks, recording the amount of force needed to do it. Because the fabric does not need to be cut into strips, the grab approach is quicker and simpler to execute than the strip method. Since only a small portion of the fabric is tested, this method might not give as precise an indication of the strength of the material.
ASTM D5034 vs ASTM D5035; Which should you choose?
The choice of grab or strip test (ASTM D5034 vs ASTM D5035) relies on the particular requirements of the test. Both the grab method and the strip method have benefits and drawbacks of their own. By understanding both methods, you can ensure that your products are suitable for the intended usage and meet the required quality standards. The strip test may be more appropriate when evaluating fabrics used in areas where strength is important, such as the production of safety equipment. On the other hand, for materials used in operations like clothing manufacturing, where speed and efficiency are critical, the grab test may be ideal.
Apparatus for ASTM D5035
- Tensile test Apparatus or Tensile Testing Machine, (Figure1) of the CRE, CRL, or CRT type design
ed for operation at a speed of 300 ± 10 mm/min (12 ± 5 in./min), preferably with a Computerized interface and interchangeable loads as required to obtain the 20 ± 3 s time-to-break. For this test method, a tensile testing apparatus with a constant extension rate is recommended. - Clamps and Jaws; each jaw face shall measure at least 10 mm (0.5 in.) wider than the specimen being tested and at least 25 mm (1.0 in.) in the direction of the applied force.
- Set the gauge length, or the distance between the clamps, to 75 ± 1 mm (3 ±05 in.).
Test Specimen’s Preparation for ASTM D5035
- As instructed in the relevant material specification, take samples from each roll or piece of fabric, and cut at least one laboratory sample the full width of the fabric and 1 m (1 yd) along the selvage (machine direction).
- When the strength of wet specimens without sizing or applied finish (e.g. water repellent) is required, before preparing the test specimens, remove the applied finish material so that it will not affect the physical properties of the fabric.
- Depending on which test you want to perform i.e., Raveled Strip Test or Cut Strip Test, cut the specimen as prescribed. The kind of clamps being used determines the specimen’s length. The specimen needs to be long enough that it extends at least 10 mm (0.5 in.) at either end and to extend through the clamps.
Testing Procedure for ASTM D5035
- Place the specimen firmly in the testing machine’s clamp. Ensure that the specimen’s tension is the same across the clamped breadth. To disperse the holding pressure over the top (front) jaw’s
clamping surface, tighten the clamps. Overly tight clamps will break the jaws at the front, while overly slack clamps will slip or break the jaws and spin at the back. (Check figure 2) - To check for specimen slippage, make a mark across the specimen at the inner front border of each jaw. The mark will shift away from the jaw edge when slippage happens.
- Run the machine until it breaks the specimen.
- Discard the result and take another specimen if the specimen slips between the jaws breaks at the edge or within the jaws, or if the result is noticeably below the average of the set of specimens for any other reason.
Conclusion and Report Formation
- Measure the average breaking force for all specimens for each laboratory sample and testing circumstance. Record each sample data separately from the computer.
- Include a summary of the product as well as the sampling technique.
- Report the specimen’s average breaking force under each fabric testing standard.
- Mention the kind of testing apparatus, strip test, and size of jaw faces used.
- Also, write about the kind of jaw padding and, if any, modified jaw faces used.
- If the size material or finish has been removed, describe the procedure.
- While making the fabric lab test report, state that Test Method D 5035 was followed in testing the specimens.
FAQs
- What do you mean by textile testing?
A definition of textile testing would be “Examining and determining the physical, mechanical, and chemical properties of a textile.” Textile testing is crucial because it can identify issues before they arise and guarantee quality.
- What is the difference between ASTM D5034 and 5035?
The difference is primarily caused by the effective width of the extended fabric. In the case of the strip method, the effective width is limited to the sample’s cut width, but in the grab method, the sample’s portion held by the jaws and the proportionate effect of the sample hanging over the jaws are included.
- What is the difference between elongation and tensile strength?
When a material is subjected to a tensile load, elongation is a measurement of the amount of change that happens prior to the material breaking. The ability of a material to bear stretching pressures before breaking is measured by its tensile strength. At break levels, materials with lower tensile strength usually exhibit increased elongation.
- Which universal testing machine working principle is used in test?
The main principles that are used in the test include constant-rate-of-load (CRL), constant rate of traverse (CRT), and constant-rate-of-extension (CRE).
- What is the tensile test purpose for fabric?
Tensile testing calculates the force required to break and extend a specimen. It helps to evaluate the elasticity and strength of various materials including woven, knitted, and nonwoven textiles.
Related Resources
ASTM D5034/ASTM D5035 Electronic Strength Machine YG(B)026HC
ASTM D5034 Electronic Strength Instrument YG(B)026G
Fabric Tensile Tester – An Ultimate Guide for Textile Manufacturers and Laboratories
ed for operation at a speed of 300 ± 10 mm/min (12 ± 5 in./min), preferably with a Computerized interface and interchangeable loads as required to obtain the 20 ± 3 s time-to-break. For this test method, a tensile testing apparatus with a constant extension rate is recommended.
clamping surface, tighten the clamps. Overly tight clamps will break the jaws at the front, while overly slack clamps will slip or break the jaws and spin at the back. (Check figure 2)