AATCC 22 Water Repellency Spray Test: Experience and Insights

Water repellency is a property of fabric that resists wetting when in contact with fluids. This test can be applied to various textile fabrics, whether having a water-repellent finish or not. This article will guide you in understanding its scope and how to perform this test in a fabric testing laboratory as directed in AATCC 22.

Water Repellency

Water Repellency can also be described as the hydrophobic nature of the fabric. It is an advanced level of water-resistant coatings. Water-repellent finishes are chemical finishes that resist the penetration of water. They are comfortable to the wearer because the fabric pores remain open. There are 3 types of water-repellent finishes.

  • Non-durable finish
  • Semi-durable finish
  • Durable finish

Non-durable finishes are usually based on paraffin wax. They are not durable as they are removed in washing. Semi-durable finishes are wax or salt solutions. They can withstand multiple washes but are eventually removed. Durable finishes can be silicone-based or with pyridinium compounds.

Nowadays, DWR (Durable water-repellent) finishes that are more breathable and provide maximum water-resistant protection are used.  Due to its breathable nature, it releases trapped moisture and prevents garments from getting stuck with the skin. This gives the wearer a more comfortable feeling and enhances athletes’ performance.

Water-Repellency Standards

In addition to AATCC-22, the following methods are used to measure fabric water repellency.

  • ISO 4920 – Determination of resistance to surface wetting (Spray Test)
  • GB/T4745 – Chinese method for measuring the water resistance of textiles by spray test
  • ISO 9073-17 – Determination of water penetration (Spray Impact)
  • AATCC 42 – Test method for Water resistance (Impact Penetration)
  • JISL 1092 – Japanese method for testing water resistance
  • WSP 80.9 – Test method for non-woven

Working Principle of AATCC 22

In this test, water is sprayed over tight fabric with no slackness in a controlled environment. After spraying, the fabric becomes wet, and different patterns are formed according to the repellent nature of the fabric. These patterns are then evaluated by comparing them with the standard chart.

Apparatus for AATCC 22

  • Spray Tester
    Spray Tester

    Spray Tester

  • Water Cylinder having 250 ml measuring capacity
  • Stopwatch/Timer
  • Distilled water having a temperature of 27 ± 1°C

Sample Preparation for AATCC 22

  • Take samples with dimensions 180 x 180 mm.
  • Take samples from different places so that no sample should have the same yarns in length or width.
  • Take a minimum of 3 samples or as per requirement.

Conditioning of Samples

  • Samples should be conditioned at standard atmospheric conditions for about 4 hours. i.e. 21 ± 1°C and 65 ± 2% relative humidity.

AATCC 22 Testing Procedure 

Fabric at 45 angle
Fabric at 45 angle
  1. Tightly fasten the sample on the specimen holder at 45°, which has a 152.4 mm diameter.
  2. The fabric should be wrinkle-free and have a smooth surface.
  3. Fabric samples should be mounted so that fabric faces should be exposed to water spray. Also, fabric orientation should be adjusted, keeping in mind the end product of the fabric.
  4. Place the hoop so that both the spray pattern and hoop are aligned and have the same center.
  5. Pour water into the funnel and wait for 25-30 sec to spray.
  6. Take the hoop by the bottom and tap it twice firmly, once at the opposite edge, and then by rotating the hoop by 180°.
  7. Pouring water in funnel
    Pouring water in a funnel

    Repeat the process again for other samples

Evaluation and Grading 

Assessment of Sample

Fabric after test
Fabric after test
  • Evaluate the sample immediately after the test.
  • Place the sample in the center of the cabinet for assessment.

Evaluation Scale 

  • Use the following spray test grading chart to assign a grade to each sample. For a rating of 50 or higher, use intermediate values if the grade is between two. e.g. 60, 75.

100 – No sticking of water droplets

90 – Slight sticking of water

80 – Wetting of specimen at spray points

70 – Partial wetting of specimen at spray points

50 – More than 80% of the surface becomes wet

  0 – Complete wetting of sample

  • Compare the fabric sample visually with the rating chart.
  • Assign the nearest rating corresponding to the chart.
  • If the pattern is in between 2 ratings, use the intermediate value. e.g., 95, 85, etc.
  • Each sample should be evaluated separately.

Report Formation

After completing the test, make a report including the following details

  • Fabric sample details (e.g. material of yarn, applied finishes)
  • Number of test samples
  • Date of test
  • Mention that the test is performed per AATCC-22.

Experience and Insights on AATCC 22

  • The sample should be taken randomly. Try samples having different yarns. i.e., take samples along the width of the fabric.
  • Always mount the fabric with its face upward or use the surface at which the finish is applied.
  • While pouring water, don’t touch the funnel with the measuring cylinder, as it can change the set position of the spray nozzle.
  • Spray time is 25-30 seconds. If time decreases or exceeds, check the nozzle holes to see if they are blocked. Adjust the nozzle accordingly.
  • Evaluate the sample immediately, as the water pattern is affected with time.

Difference between Water Resistant, Water Repellent and Water Proof Fabrics

Water Resistant

This is the entry-level protection from water and the most basic form of protection in the repellent category. Manmade fibers like polyester and nylon are hydrophobic and are usually used in fabric with a higher cover factor and resist water entering through the fabric. The cover factor determines the density of a fabric. If a fabric has a high density and compact fabric structure, it takes time for water to pass through the fabric.  Garments with water resistant tags are not meant to deal with continuous exposure to extreme weather, instead they can withstand light water contact like slow rain showers.

Water Repellent

This is a higher level of fabric impervious to water than water resistant. Water in the form of beads remains in fabric due to its hydrophobic nature. A fabric can be made water-repellent by adding a coating or finishing of hydrophobic material. These fabrics have nearly same performance as waterproof fabrics

This is the best option for athletes as it is more breathable, effective, lightweight, and comfortable than waterproof fabrics.

WaterProofness

In this stage, a garment is completely immune to water. These garments have tight stitching, synthetic fibers, and chemical coatings, along with additional layers of protection under seams and zippers. They are made for special environments like in snow, heavy rainfall and tents, where complete water protection is required. Due to their impervious nature, these fabrics are also used in dive suits requiring submersion. These fabrics have less comfortability than water-repellent fabrics.

It is also important to understand that, despite a garment’s label indicating its repellency category, its performance depends on the material’s quality, structure, and chemical finish. Also, there are different tests like spray tests, rain tests, and hydrostatic tests, each having different rating techniques and test methods.

Conclusion 

In conclusion, the water repellency test plays a great role in the comfortability and breathability of the fabric. This test ensures that the fabric remains dry and the wearer feels comfortable in humid environments. This test also shows the effectiveness of water-repellent finishes applied on fabrics.

FAQs

  1. What is the Bundesmann water repellency test?

This test evaluates a fabric’s ability to withstand rain, such as in raincoats. A simulation of the storm effect is produced in the fabric testing laboratory. It is based on ISO 9865.

  1. What factors affect water repellency?

It depends on the nature of fibers, whether they are hygroscopic or hydrophobic. Applied finishes on fabric also affect water repellency.

  1. How can a fabric be made water-repellent?

Normally, finishes or coatings are applied for this purpose. These coatings

layer over the fabric, restricting water from moving inward.

  1. What is the difference between water-resistant, water-repellent, and waterproof?

Water-resistant means a material is capable of partially resisting water. Water-repellent means water is difficult to penetrate due to coatings or surface layers. The waterproof material is completely immune to water.

  1. What are the uses of Spray Tests?

It can be used to evaluate fabrics’ resistance to water. Daily use items like backpacks, tents, and outdoor wear can be tested for performance.

Related Resources

Water Repellency Tester

ISO 4920 Water Repellency Tester Y(B)813

AATCC 35 Fabric Waterproof Performance Tester Y(B)813G

Bundesmann Test

    Scroll to Top

    ASK FOR A QUOTE

    We will contact you in one working day. Please pay attention to the email with suffix @darongtester.com