Liquid Moisture Management Test Method AATCC 195 measures, evaluates and classifies liquid moisture in textile fabric or articles. It is used for all textile materials, such as knitted, woven, and non-woven fabric or microfiber. Characteristics such as repulsion, attraction, and resistance-based results can be achieved using this method. It can also evaluate the results of yarn and fabric or articles.
AATCC 195 Equipment
To perform this Liquid Moisture Management Test, we will need:
- A moisture tester;
- A computer with moisture management properties software installed,
- Distilled water;
- 9% of NaCl (Sodium chloride) solution;
- Conductivity meter;
- AATCC bolting paper
AATCC 195 Sample Preparation
1. To make a testing specimen, Wash the testing specimen according to AATCC LP1 laboratory procedure while using a washing machine and keep the conditions as instructed in AATCC LP1 home laundering or as agreed on washing between purchaser and supplier.
2. Cut five 8×8 cm testing specimens diagonally widthwise of the sample.
3. Place the specimen tension-free on a flat, smooth surface, and the conditioning of the sample room should be 21 ± 2°C (70 ± 4°F) and 65 ± 5% RH as instructed in ASTM D1776.
AATCC 195 Test Procedure
1. Dissolve 9 grams of sodium chloride ( NaCl ) in 1L of distilled water to prepare 9 % of the solution.
2. Adjust the electrical conductivity of the solution to 16± 0.2milli Siemens at 25°C. Add sodium chloride or distilled water to get 16± 0.2milli Siemens electrical conductivity.
3. Follow the DaRong instructions written in the use manual for preparing the testing instruments.
4. keep the upper sensor locked and place a paper towel on the lower sensor. Press the “Pump” button for 1 min to 2 min until the required amount of test solution is drawn from the solution container and drips onto the paper towel, and there shouldn’t be any air bubbles inside the tubing. Remove the paper towel.
5. Place the ready testing specimen on the lower sensor.
6. When the sample is completed, rest, release the upper sensor & shut the door.
7. The percent water content graph should be zero for every specimen.
8. Set the measure time for 120 seconds and start the test.
9. After 120 seconds, the software automatically stops and calculates our results.
AATCC 195 Test Report
For the tested sample, take the average values for each measurement unit as follows:
Wetting Time – WTT (top surface) and WTB (bottom surface), Absorption Rate – ART (top surface) and ARB (bottom surface), Maximum Wetted Radius – MWRT (top surface) and MWRB (bottom surface), Spreading Speed – SST (top surface) and SSB (bottom surface), Accumulative One-way Transport Capability – (R), and Overall (liquid) Moisture Management Capability. To summarize, the below table must be used for grading.

FAQs
What is the moisture management test method?
This is the method in which a specific quantity of solution is dropped on the center of the upper surface of the testing specimen, which may be knitted, woven, or nonwoven.